Pipe carries every fluid between the machines the other chapters cover, and its joints are where most leaks start. What a line is made of, how it is joined, and what its gasket and bolts can take decide whether your repair holds.
Lessons teach one thing step by step. Simulators are free play: best after the lesson.
Maker’s values override these.
| Point | Typical |
|---|---|
| Seawater velocity in 90/10 Cu-Ni | ≤ 3 m/s |
| Galvanized steel, hot fresh water | Below about 60 °C — above it the zinc stops protecting |
| GRP pipe | Up to about 80 °C; resin maker's figure |
| PVC drain and sanitary | Below about 60 °C; no steam |
| Flange faces before bolting | Parallel within about 1 mm; holes line up without bars |
| Socket-weld gap at receptacle bottom | About 1.5 mm |
| Bolt thread past the nut | 1–3 full threads |
| Flange torque | Star pattern, 30 % · 60 % · 100 %, then once round at 100 % |
| Hydrotest after repair, pressure piping | Typically 1.5 × design, held while every joint is walked |
| Support spacing, steel, water-filled (shore guide; ships closer) | DN25 ~2 m · DN50 ~3 m · DN100 ~4 m |
Each one is a set of readings. Decide what they mean and what you’d check first, then look.
| Symptom | Check first | Likely causes | Action |
|---|---|---|---|
| Pinhole on a seawater bend or just downstream of a valve | Wall at the outside of the bend | Erosion — velocity, throttling, high-speed GS pumping | Clamp; renew the spool; pump in low speed |
| Rust stain or wet patch on lagging | Strip the lagging there | Corrosion under wet insulation | UT the wall; renew pipe; re-lag dry |
| Steel bolts thin and scaly on a Cu-Ni or bronze flange | Bolt material | Galvanic — steel is the anode | Stainless or bronze bolts; insulating kit where specified |
| Small-bore line cracked at a fitting near an engine | Support near the tee | Vibration fatigue | Support it or fit a hose; renew the fitting |
| Flange leaks after a new gasket, worse hot | Faces parallel? Gasket type? | Pulled in by bolts; wrong gasket for the heat; not re-torqued | Realign; right gasket; retorque cold |
| Heater flange leaks on a cold start, stops warm | How fast steam went on | Gasket relaxed while cold; thermal shock | Warm through slowly; renew if it repeats |
| Cast-iron flange cracked at a bolt hole | Partner flange face | Raised face on flat face; over-torqued | Full-face gasket; cast-iron torque; replace |
| Threaded joint leaks through more sealant | Thread forms | NPT on BSPT; parallel thread without a washer | Match parts; washer or O-ring |
| Compression fitting weeps; tightening doesn't cure it | Tube bottomed? Ferrule brand? | Not bottomed; mixed makers; over-tightened | New ferrule, tube cut square and bottomed |
| Bellows bulging or weeping | Tie rods; alignment; length | Inner ply failed; thrust on flanges; misaligned | Nip up for tonight; replace; fit the rods |
| Pressure on a "dead" line, pumps stopped | Boundary valves; drain cracked | Valve letting by; trapped pressure; sea head | Third valve; bleed; watch it stay at zero |
| Pipe springs when a flange is broken | Supports either side | Unsupported run; strain locked in at fit-up | Support; refit without forcing |
| New spare won't fit — holes or bolt circle wrong | Stamps on both flanges | Different standard or rating | Adapter spool; drill only where class allows |
| Air system losing pressure fast, compressors stopped | Rate of fall; soapy water | Fitting and hose leaks; drain traps passing | Fix the leaks before blaming the compressor |
Draft: this page is drawn from the book manuscript and is still being checked.