← Welding and Cutting · Lesson: Weld a Bracket · Weld Test Positions · Welding Symbols
What you need at the bench before you strike an arc: which rod, what size, how many amps, which way round the leads go, what shade, and whether to preheat. Plus what the rod number means, what the metal is, and how hard it is.
Mark anything that's true. Any mark and it isn't a ship's-staff weld today.
Stick rods print it on the flux near the bare end. Try a few:
| Part | Steel stick rod | What it says |
|---|---|---|
| E | E7018 | Electrode (stick). ER = wire or filler rod. B = brazing filler |
| 70 | E7018 | Weld metal tensile, thousands of psi (ksi). Five digits: the first three (E11018) |
| 1 | E7018 | Positions: 1 all, 2 flat and horizontal fillet, 4 all with vertical down |
| 18 | E7018 | Last two together: the flux and the current it runs on |
| -1 H4 R | E7018-1 H4R | Extras: tougher in the cold, low hydrogen level, moisture-resistant flux |
Stainless reads differently: E309L-16 is the alloy, then L for low carbon, then the flux and current.
Answer what you can; skip what you can't. The list on the right narrows as you go. Grind a clean spot first: paint, scale and plating lie.
Shop tests sort families, not grades. Where it matters (pressure work, class repairs, an alloy you can't name), the answer is the drawing, the parts list, the mill certificate, or a PMI gun (XRF) from the yard or a surveyor.
A good, sharp file. Pick a spot that won't matter, take off any scale or case, and stroke once with steady pressure. How did it feel?
Type into any box. Steel only, approximate; a converted number is an estimate, not a measurement.
Typical; the WPS or the rod maker's sheet overrides. Start mid-range flat; about 10% less vertical and overhead. Rule of thumb: about 1 A per thousandth of an inch of core (1/8 in = 0.125 in ≈ 125 A).
| Rod diameter | E6010 / E6011 | E7018 | Stainless (-16) |
|---|
Not on the chart (E6013, E7024, nickel, hardfacing): the range is printed on the box. Use it.
| Setting | Also called | Electrode lead on | What it does | Used for |
|---|---|---|---|---|
| DCEP · DC+ | Reverse polarity | + terminal | Deepest penetration with stick; steadiest arc | E7018, E6010, E6011, stainless rods, MIG solid wire, gas-shielded flux-core |
| DCEN · DC− | Straight polarity | − terminal | Rod melts off faster, shallower; with TIG most of the heat goes into the work | TIG on steel and stainless, self-shielded flux-core (E71T-11), E6013 on thin sheet |
| AC | – | Either | Flips 120 times a second at 60 Hz; no arc blow | AC-only sets with E6011, E6013 or AC-rated E7018; TIG on aluminum |
Work clamp on the other terminal, on bare metal of the part, close to the joint. Never through a bearing, gearbox or control module.
OSHA minimum, and the ANSI/AWS starting point. Start dark and go lighter until you can see the puddle, never below the minimum.
| Job | Size or amps | Min | Suggested |
|---|
| Joining | Stick | MIG wire | TIG rod | Notes |
|---|---|---|---|---|
| Mild steel, load-bearing | E7018 | ER70S-6 | ER70S-2 / -6 | Rods from the oven |
| Mild steel, rusty or a root in an open gap | E6010 / E6011 | E71T-11 | – | E7018 fill and cap over it |
| Thin sheet, guards, tacks (not for load) | E6013 | ER70S-6, small wire | ER70S-2 | |
| 304 to 304 | E308L-16 | ER308LSi | ER308L | Own brush and discs |
| 316 to 316 | E316L-16 | ER316LSi | ER316L | Seawater grade |
| Stainless to mild steel, or stainless you can't name | E309L-16 | ER309LSi | ER309L | Never E308L or E7018 here |
| Duplex (2205) | E2209-16 | ER2209 | ER2209 | Qualified welder; ask the engineer in charge |
| Cast iron | ENi-CI | – | – | Short runs, peen; or braze |
| Copper, brass, bronze to each other or steel | Braze: BCuP (copper to copper, no flux), BAg silver (anything to anything, with flux), bronze rod for cast iron | See Brazing in the chapter | ||
| Cu-Ni, aluminum | Send out | Not a shipboard stick job | ||
| Number | Read it as |
|---|---|
| ER70S-6 | ER wire or rod · 70 ksi · S solid · 6 = most manganese and silicon to clean up mill scale and light rust. The common MIG wire. DCEP with gas |
| ER70S-2 | Extra deoxidizers (aluminum, titanium, zirconium): the usual TIG rod for steel |
| E71T-1C / -1M | E · 70 ksi · 1 all positions (0 = flat and horizontal only) · T tubular · 1 = gas-shielded, DCEP · C 100% CO₂, M argon-CO₂ mix |
| E71T-11 | Self-shielded (no gas bottle), DCEN, works in a draft. Heavy fume: extraction |
| ER308LSi | Stainless MIG wire, L low carbon, Si extra silicon so the puddle wets out |
| Tungsten (TIG), by the painted tip: green pure (AC on older sets) · red 2% thoriated (slightly radioactive: don't breathe the grinding dust) · gold 1.5% and blue 2% lanthanated (AC or DC, the modern all-rounder) · gray (older boxes orange) 2% ceriated · brown or white zirconiated (AC). Check the box: makers' colors don't all agree. | |
| Steel | Preheat |
|---|---|
| Mild steel, cold or damp | Warm to hand-hot, about 40 °C, to drive off moisture |
| Mild steel over 20 mm (¾ in) | The WPS. As a floor, AWS D1.1 asks at least 10 °C with low-hydrogen rod up to 38 mm, and 65 °C with E6010 / E6011 |
| Cast iron | Nickel rod in short runs with no preheat, or preheat evenly to about 250–300 °C and cool slowly, wrapped |
| Stainless | None. Keep it hand-hot or cooler between passes |
| Hard or alloy steel | By carbon equivalent, below. Prove it with temperature crayons, not by feel |
IIW: CE = C + Mn/6 + (Cr+Mo+V)/5 + (Ni+Cu)/15. Percent by weight; leave blank what isn't listed.
| Oxy-acetylene job | Oxygen | Acetylene |
|---|---|---|
| Brazing or welding, small tip | 0.3–0.7 bar · 5–10 psi | 0.3–0.5 bar · 5–7 psi |
| Cutting plate to 25 mm | 2–3 bar · 30–45 psi | 0.3–0.5 bar · 5–7 psi |
| Rod size | 1/16 | 5/64 | 3/32 | 1/8 | 5/32 | 3/16 | 1/4 |
|---|---|---|---|---|---|---|---|
| mm | 1.6 | 2.0 | 2.4 (2.5) | 3.2 | 4.0 | 4.8 (5.0) | 6.4 |
A sound weld: even width and ripples, face flat to slightly convex, toes blending into both plates, legs equal and to size on the gauge, no holes or cracks.
| Defect | Looks like | Means | Fix |
|---|---|---|---|
| Porosity | Pinholes, worm holes | Damp rod; long arc; dirt, paint, zinc; draft on gas-shielded wire | Grind out, clean, dry rods, shorter arc |
| Undercut | Groove melted into the plate at the toe | Amps high; travel fast; no pause at the toes | Blend if shallow; else a small stringer, lower amps |
| Cold lap | Bead sitting on the plate, crevice at the toe | Amps low; travel slow; puddle ahead of the arc | Grind out; re-weld hotter |
| Slag inclusion | Dark lines or pockets between runs | Slag left from the last pass; amps low | Grind out; chip every pass |
| Lack of penetration | Unfused root on the back of a butt | Gap tight; no bevel; amps low | Back-grind; weld the back |
| Cracking | Down the center, along the toe, or a crater star; may show hours later | Damp rod; fast cooling; restraint; cast iron; crater not filled | Grind all of it out, prove with dye penetrant; preheat, dry rod, fill craters |
| Burn-through | Holes through thin plate or the root | Amps high; gap wide; travel slow; rod too big | Lower amps, smaller rod; fill from the edges |